I'm trying to bond two 17”x17” aluminum plates with 3M AF163-2 structural adhesive. The plates are modified sulfuric acid anodized, primed with 3M EC 3960 adhesive primer within 4 hrs. after anodization , adhesive film applied and cured 250F/ 45psi 90min.
Lap shear test per ASTM D1002 gives 4700-5000psi but climbing drum peel test ASTM 1781 gives VERRRY bad results (4-5 lb/in) or very good . . . 80-85 lb/in. The worst is that on the same plate from which I cut 5 test samples I may have 3 disastrous failures and 2 strong bonds . . . I can't understand what is happening. There aren't medium values . . . it fail miserably or it pass far high on the same panel.
I have read Boeing, Bombardier and DeHavilland specifications concerning metal bonding and I suppose that every little detail is controlled, adhesive primer is cured, no contamination, I have plates from 2 supplier, anodized in 2 different shops . . . I already run around 40 tests pieces i don't know what to do anymore.
Does anybody has heard about such contrary comportment on samples cut from the same panel?
What I'm doing wrong? Does anodization process lives residues on plates?, or hydration after anodization may developed a kind of local shield so fast???
Lap shear test per ASTM D1002 gives 4700-5000psi but climbing drum peel test ASTM 1781 gives VERRRY bad results (4-5 lb/in) or very good . . . 80-85 lb/in. The worst is that on the same plate from which I cut 5 test samples I may have 3 disastrous failures and 2 strong bonds . . . I can't understand what is happening. There aren't medium values . . . it fail miserably or it pass far high on the same panel.
I have read Boeing, Bombardier and DeHavilland specifications concerning metal bonding and I suppose that every little detail is controlled, adhesive primer is cured, no contamination, I have plates from 2 supplier, anodized in 2 different shops . . . I already run around 40 tests pieces i don't know what to do anymore.
Does anybody has heard about such contrary comportment on samples cut from the same panel?
What I'm doing wrong? Does anodization process lives residues on plates?, or hydration after anodization may developed a kind of local shield so fast???